Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the all-in-one-seo-pack domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /data/wwwroot/wordpress/wp-includes/functions.php on line 6114

Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the unlimited-elements-for-elementor domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /data/wwwroot/wordpress/wp-includes/functions.php on line 6114

Notice: Function _load_textdomain_just_in_time was called incorrectly. Translation loading for the js_composer domain was triggered too early. This is usually an indicator for some code in the plugin or theme running too early. Translations should be loaded at the init action or later. Please see Debugging in WordPress for more information. (This message was added in version 6.7.0.) in /data/wwwroot/wordpress/wp-includes/functions.php on line 6114
低成本固相法合成 Na–β”-Al2O3固体电解质陶瓷 - 宏赫化工 宏赫化工

宏赫化工

探索氧化铝的世界

固相法合成 Na–β"-Al2O3固体电解质陶瓷

王竹梅,张天峰,左洪威,谢志翔,李月明,程亮

以工业氧化铝为原料,采用低成本埋烧工艺,用传统固相法制备Na-β"-Al2O3相相对含量高的固体电解质陶瓷材料。采用综合热分析仪、X射线衍射以及扫描电子显微镜对样品进行表征,采用交流阻抗法测试了样品的电导率。结果表明:βʺ-Al2O3相的相对含量与配方Na1.67(1+x)Li0.33Al10.67O17中的Na含量和合成温度密切相关,陶瓷在x=0.15、烧结温度为1580℃时,βʺ-Al2O3相的相对含量最高,达97.19%,此时陶瓷的微观结构较致密,300℃的电导率为0.028S/cm、电导活化能为0.259eV。该方法制备工艺简单、适合工业大规模生产。
βʺ-Al2O3 Solid Electrolytes

进入21世纪以来,能源问题成为了世界各国关注的焦点,钠硫电池作为一种新型的储能电池,因其具有比能量高、放电功率大、无自放电、成本低、无污染等诸多优点而成为研究热点。钠硫电池的性能取决于其固体电解质β”-Al2O3的性质,因此,β”-Al2O3电解质的制备和性能研究也逐渐成为备受重视的研究领域。

β″-Al2O3是一种复杂的钠铝复合氧化物,经验式为Na2O·5.33Al2O3,它还有另外一种同质异构物β-Al2O3,经验式为Na2O·11Al2O3。β″-Al2O3的电导率是β-Al2O3的数10倍,但在Na2O-Al2O3体系中往往同时存在β-Al2O3与β″-Al2O3两种晶相,且在高温烧结过程中,β″-Al2O3相极易向β-Al2O3相转变,因而,想要制得β″-Al2O3相含量高的固体电解质材料较为困难。

传统合成β”-Al2O3的主要方法是将高纯α-Al2O3、Na2CO3及少量稳定剂如MgO或Li2O等混合,在1580℃以上的高温下烧结而成,此法因使用高纯α-Al2O3原料使得成本较高。近十几年来,出现了一些关于采用新式化学方法如溶胶-凝胶法、醇盐水解法、溶剂燃烧法、共沉淀法法等制备β”-Al2O3的相关报道,这些合成方法具有合成材料纯度高、分布均匀、烧结温度低等优点,但其合成工艺较为繁杂、设备和操作要求较高,相对于传统固相法难以工业化大生产。另外,由于Na2O在高温烧结时极易挥发,因而无论采用传统固相法还是新式化学法制备β″-Al2O3,为了保证陶瓷烧结后的性能,往往在素坯烧结时,均需将素坯埋入预合成的前驱体中进行埋烧,这样的埋烧工艺使得生产成本大幅增加。

采用固相合成法,使用低成本的工业级α-Al2O3(纯度为82.90%,主要杂质为结晶水)为原料,同时改进埋烧工艺,将埋烧料分为两部分,一部分为少量的预合成前驱体,另一部分为大量的工业级α-Al2O3,从而降低埋烧成本,埋烧示意图见图1,探索了钠含量和烧成制度对β″-Al2O3相含量的影响,获得了性能较好的配方组成及烧成制度,该制备方法成本低,易于工业化大量生产,具有很好的应用价值。

 

1 实验

1.1 样品制备

采用工业级Al2O3、分析纯Na2CO3、分析纯Li2CO3为原料,按照Na1.67(1+x)Li0.33Al10.67O17(x=0,0.10,0.15,0.20)的化学计量比配料。将称好的原料置于球磨罐中,以无水乙醇和ZrO2球磨子为球磨介质球磨12h。将球磨好的浆料烘干后在1100℃预烧2h,将预烧后的粉料用研钵粗磨后置于球磨罐中二次球磨12h,烘干,过筛后加入质量分数为3%的聚乙烯酸缩丁醛(PVB)黏结剂造粒,等静压机下压制成直径为13mm、厚度为1.3mm左右的圆柱体。排胶后在不同的烧结温度下煅烧,保温30min,随炉冷却至室温。

1.2 样品表征用S-4800场发射扫描电子显微镜观察样品的形貌,工作电压3kV。用AXSD8ADVANCE型X射线衍射仪(XRD)检测样品的晶相组成,工作电压40kV,电流40mA,CuKα(λ=0.15418nm),扫描角5°~70°。用DT-50型热分析仪(SHIMADZU,JAPAN)检测一次球磨后粉料的热物理性能,氦气氛,升温速率10℃/min,温度范围室温~1400℃。用交流阻抗谱测试技术在CHI604C电化学测试站上测试样品的电导率,样品抛光后两面被烧银电极,用银丝引出作为电极引线,测试温度范围250~700℃,测试频率范围为10-1~105Hz,交流输入信号为10mV。

 

2 结果与讨论

2.1 热物理性能分析

为了研究粉料在不同温度下所发生的热物理变化,将一次球磨后x=0.15的粉料进行了差热-热重(TG-DTA)测试,如图2所示。由图2可见,在110.8℃处有1个明显的吸热峰,同时在TG曲线上伴随着质量的剧烈损失,这可以归结为游离水和残余乙醇的挥发;在224.4℃出现了1个微小的吸热峰,同时伴随着质量的快速减少,这可能是原料中含有的少量结晶水脱水所致;在345.6℃出现了1个明显的放热峰,同时伴随着质量的减少,这可能是粉料中残留的乙醇等有机物燃烧所造成的;在740.9℃处有1个明显的吸热峰,同时伴随着质量的快速减少,这是由于粉体中Na2CO3、Li2CO3发生分解反应,分解为Na2O、Li2O并放出CO2所致;在900~1250℃区间有1个缓慢的放热峰,质量损失并不明显,这是由于α-Al2O3与Na2O、Li2O反应形成βʺ-Al2O3、β-Al2O3、NaAl5O8和LiAl5O8所致。另外,由800~1400℃区间的TG曲线可见,虽然质量损失不明显,但仍可观察到质量缓慢的匀速减小,质量损失约为1.21%,这可归结于Na2O的挥发,由于质量损失少,并未观察到吸热峰。由于TG-DTA分析具有一定的滞后性;同时,参考其他相关文献,将预烧温度设定为1100℃。

 

βʺ-Al2O3 Solid Electrolytes

图 2 Na1.67(1+x)Li0.33Al10.67O17(x=0.15)陶瓷原料的 TG–DTA 曲线

 

2.2 XRD分析

图3为不同配方粉体在1100℃预烧后制得前驱体的XRD谱。从图3可以看出,所有样品均观察到βʺ-Al2O3和NaAl5O8特征峰,且均未观察到α-Al2O3和β-Al2O3相衍射峰,说明该预烧温度下,原料中的α-Al2O3几乎已经完全反应,且此时β相含量很少,不能在XRD谱观察到;同时,XRD谱中出现了3个未知峰,可能是一些复杂的Na、Al、O化合物;当x=0和x=0.1时,XRD谱中βʺ-Al2O3和NaAl5O8相所对应的衍射峰较宽、衍射峰强度较低,表明产物结晶度不高;当x值逐渐增大至0.15和0.20时,βʺ-Al2O3和NaAl5O8特征峰明显增强且尖锐,表明随着Na2O的升高,粉体预烧后结晶度提高,晶相发育更趋完善。

 

βʺ-Al2O3 Solid Electrolytes

图 3 1 100 ℃预烧后各前驱体样品的 XRD 谱

 

图4为不同配方前驱体经压片制样后在1580℃下煅烧后的XRD谱及βʺ-Al2O3和β-Al2O3标准图谱。由图4可以看出,所有样品均为βʺ-Al2O3相和β-Al2O3相,且随着x值即Na2O含量的增加,其βʺ-Al2O3特征峰在2θ=45.9°的峰强呈先增大后减小的趋势。分别选取2θ=44.5°(β-Al2O3)和2θ=45.9°(βʺ-Al2O3)特征峰,根据式(1)[12]可计算出βʺ-Al2O3相的相对含量,结果如表1所示。由表1可见,βʺ-Al2O3相的相对含量随着配方中Na2O含量的提高呈先增加后减少的趋势,x=0.15时最大,达97.19%;当Na2O含量稍提高至x=0.20时,βʺ-Al2O3相的相对含量急剧降低至75.66%,此时可观察到明显的β-Al2O3相衍射峰(见图4,x=0.20,2θ=44.5°),这可能是由于Na2O含量过高,导致预烧时生成过多的NaAl5O8,而在烧结时没有足够的LiAl5O8与之反应生成βʺ-Al2O3相,从而生成了更多的β-Al2O3相。

βʺ-Al2O3 Solid Electrolytes

其中:Iβ、Iβʺ分别为β-Al2O3与βʺ-Al2O3的特征峰强度。

 

表 1 不同配方样品在 1 580℃煅烧后 βʺ-Al2O3相的相对含量

βʺ-Al2O3 Solid Electrolytes

 

βʺ-Al2O3 Solid Electrolytes

图 4 各样品在 1 580 ℃煅烧后的 XRD 谱

 

图5为x=0.15样品分别在1560、1580、1600℃煅烧后的XRD谱。采用式(1)相同的方法计算βʺ-Al2O3相的相对含量,如表2所示。由图5特征峰放大对比图结合表2可以看出,在1560℃烧结时,样品βʺ-Al2O3相所对应的特征衍射峰的强度较低且半峰宽较宽,说明结晶度不高,但βʺ-Al2O3相的相对含量较高,为92.02%;在1580℃时,衍射峰的强度最高且尖锐,说明该温度下晶体的结晶度最好,βʺ-Al2O3相的含量也最高,为97.19%;而在1600℃时,出现了明显的β-Al2O3相特征峰(2θ=44.5°),βʺ-Al2O3相的相对含量也下降到了66.09%。这可能是2个方面的原因造成的,一是随着温度的进一步增高,βʺ-Al2O3相向β-Al2O3相转变;二是随着温度的升高,Na2O挥发加剧,导致样品向Na含量更少的β-Al2O3相转变。

 

βʺ-Al2O3 Solid Electrolytes

图 5 不同温度煅烧后 Na1.67(1+x)Li0.33Al10.67O17(x=0.15)陶瓷的 XRD 谱

 

2.3 微观形貌分析

βʺ-Al2O3 Solid Electrolytes

图 6 不同温度烧结后 Na1.67(1+x)Li0.33Al10.67O17(x=0.15)陶瓷断面的 SEM 照片

 

图6为x=0.15样品在不同温度煅烧后的SEM照片。从图6a可以看出,样品在1560℃煅烧后仍有少量气孔,且可观察到大量的熔融态物质,结合图4可知此时样品结晶度较低;从图6b可以看出,样品在1580℃煅烧后,样品表面的晶粒尺寸较小,晶粒间有微小的尺寸差距,晶界也较为明显。从图6c可以看出,1600℃时,几乎已经观察不到晶界的存在,晶体最致密,但结合图5和表2可知,此温度下βʺ-Al2O3相的相对含量反而最低,这非常不利于Na+的传导。

表 2 x=0.15 配方不同烧结温度 βʺ-Al2O3相的相对含量

βʺ-Al2O3 Solid Electrolytes

 

2.4 电导率分析

用交流阻抗仪测试了1580℃烧结后、x=0.15样品在不同温度下的交流阻抗图谱如图7所示;其中300℃的交流阻抗谱如图7中的插图A所示,求得不同温度下的电导率如图7插图B所示。由图7可以看出,随着温度的升高样品的电导率逐渐提高,样品在300℃的电导率为0.028S/cm。

 

2.5导电机制分析

由Arrnhenius理论导出电导率与温度相互关系[14]结果如式(2)所示。式中:A为特征常数;R为摩尔气体常数;Ea为电导活化能,包括缺陷形成能和离子迁移能。将式(2)两边取对数得式(3),将不同温度下的电导率代入式(3),得到样品的电导率和温度关系曲线如图8所示。从图8可以看出,曲线几乎为线性,由此求出晶体的电导活化能为Ea=0.259eV。

 

βʺ-Al2O3 Solid Electrolytes

图 7 Na1.67(1+x)Li0.33Al10.67O17(x=0.15)陶瓷在 250~700 ℃的交流阻抗谱

 

βʺ-Al2O3 Solid Electrolytes βʺ-Al2O3 Solid Electrolytes

 

βʺ-Al2O3 Solid Electrolytes

图 8 Na1.67(1+x)Li0.33Al10.67O17(x=0.15)陶瓷电导率和温度关系曲线

 

根据样品在300℃测量的交流阻抗谱线(Measuredvalue),参考Zhu等的研究成果[15],绘制等效电路模型如图9中插图所示,用zsimdemo软件进行拟合,得到拟合谱线(Fittedvalue)见图9,对比2条谱线可见,2条线几乎重叠,说明等效电路模型与实际电路相近。等效电路模型中,L1(Inductanceduetosilverwireandsilverelectrode)和R0(Leadwireresistance)分别为银丝和银涂层的电感和电阻;CPEg(graincapacitance)和Rg(grainresistance)分别为晶粒的电容和电阻;CPEgb(grainboundarycapacitance)和Rgb(grainboundaryresistance)分别为晶界的电容和电阻;CPEdl(adoublelayercapacitance)为双层结构电容;Rct(chargetransitionresistance)为电荷转移电阻,由于多晶陶瓷电解质的性质,纯电容在这里被一个角向量元件(CPE)所取代。

 

βʺ-Al2O3 Solid Electrolytes

图 9 Na1.67(1+x)Li0.33Al10.67O17(x=0.15)陶瓷在 300 ℃下的拟合电路交流阻抗谱

 

3 结论

1)1100℃预烧已形成部分βʺ-Al2O3,且配方Na1.67(1+x)Li0.33Al10.67O17中的Na含量越高,βʺ-Al2O3相的晶相发育越完善。

2)βʺ-Al2O3相的相对含量与配方Na1.67(1+x)Li0.33Al10.67O17中的Na含量和合成温度密切相关,陶瓷在x=0.15、烧结温度为1580℃时,βʺ-Al2O3相的相对含量最高,达97.19%,此时陶瓷的微观结构较致密,300℃下的电导率为0.028S/cm、电导活化能为0.259eV。